Coldwork and Slump

With the bowl “blank” fired, the last steps are to clean it up and slump it.  At this stage you have several options (which can be used in combination):

  • Trim the edges with the tile saw to clean and straighten them.
  • Cut or grind the corners to round them.
  • Sandblast the surfaces to “scrub” them clean.
  • Fire polish the piece to bring the front to a high gloss.
  • Smooth the front and/or back with either a flat lapidary grinder or diamond hand pads (as shown here:

Coldworking fused glass with diamond hand pads.

Place the piece on your chosen slumping mold, as shown in here:

Ready to slump our fused glass bowl.

Slump with the following schedule:

SEG RAMP F/H TARGET HOLD Notes
1 200 1000F If you have a shallow kiln, where the heating elements are less than 6 inches from the top of the glass, consider slowing this segment down to avoid thermal shock.
2 100 1200F A slow, steady ramp to 1200 will allow for even heating and, consequently, even slumping.
3 FULL 960F 2 hrs Anneal soak
4 100 700F Anneal cooling
5 300 100F Final cooling


That’s it - your bowl is complete!  Don’t be surprised if you find yourself looking at your scrap fusible glass in a whole new way!

Amazing Piece!

As usual, you have made something remarkable, and given clear instructions, to boot!  Thank you.  I can't wait to try this as soon as my fall shows are over, and I can start making stuff for myself again.  Wink

 

Sheryl

I was just looking at my

I was just looking at my scrap pile the other day thinking....sheesh, what am I going to do with all of that! Great tutorial.

Poppy

http://groovyglassgirl.etsy.com

Comment viewing options

Select your preferred way to display the comments and click "Save settings" to activate your changes.