Copper Inclusion: How to keep the shine?

I like to use copper sheeting and wire for inclusions in my pendants and plates. Is there a recipe for a "glaze" that can be painted on so that the copper will maintain it's glowy shine during fusing rather than dull to a red color? If not, does anyone have a suggestion on what product to buy? Just for fun, are there solutions that can be painted on that will change the color of metal inclusions? Experimentation is so fun.

I've heard that you can

I've heard that you can spray it with Super Spray before putting it between the glass.  I've never tried it so can't confirm it works but I've had it filed in the back of my brain for a while.

Terry Curtis

Try this

To keep the copper from going red, try this:

1. Prepare your copper shape/inclusion by pickling it in lemon juice; it works faster and better if the pickle is warm. The pickling will clean the copper of oils. Fifteen minutes works best for me. I usually have a small crockpot of the pickle solution going. (There are commercially available pickles, but lemon juice does work for the small bits and pieces I use, it's not as caustic, it's cheap and it's at the grocery.)

2. Remove items from pickle using tweezers. Dry. Paper towels work fine-- a hair dryer if you're in a hurry. Use tweezers in handling the copper to prevent putting oils back on the cleaned copper.

3. Coat with Super Spray. I give it at least two coats on both sides. Paint it on in one direction, then paint perpendicular to the first set of paint strokes. Or you can spray the solution-- you might be able to get away with one coat. Take precautions if you do spray.

4. Place your dried inclusions within your design and fire away.

This has worked for me pretty regularly. I've sometimes put items into the kiln and discovered that I hadn't done a great job of coating something and have gotten red streaks. Sometimes it looks very cool -- duotoned copper! Sometimes not so much.

There's a recipe for devit spray on this site that might work with copper, but I haven't tried it.

If you do pickle more than one thing at a time, I've found that it works better if they aren't touching one another in the pot. And if you don't want to invest in a small crock pot (I got two at the Goodwill for a buck each), then just set the container with the lemon juice inside another container with hot water.

Have fun!

 

 

 

 

 

 

 

Just a question. Would

Just a question.

Would cleaning the copper with steel wool and then washing work also?

Steve

 

Stephen Richard

blogs at: http://www.verrier-glass.blogspot.com/   and  http://www.glasstips.blogspot.com/

Probably

The steel wool and elbow grease will probably work as long as you get the copper nice and shiny and free of oils. But the problem is that you cannot see with the naked eye whatever oils are left. Oils will prevent the Super Spray or Spray A from adhering to the copper and allow the copper to come in contact with the glass and react to it.

I work mostly with foils and small bits of wire so pickling is far more time-effective than scrubbing.