I had a firing schedule to slump wine bottles over 9 years ago and lost it. Does anyone have one to share, I have a Paragon GL24ADTSD for my fusing kiln. Thanks, Melody in Arizona


Firing schedules
Paul has a number of firing schedules on this site. Go to "tools" on the top bar, find firing schedules and you will see a number of purpose based schedules. Remember that bottles behave very much like float glass.
Stephen Richard
blogs at: http://www.verrier-glass.blogspot.com/ and http://www.glasstips.blogspot.com/
Wine Bottle Firing Schedule
600 1100 10
300 1300 30
AFAP 1425 5 to 15
AFAP 1000 10
180 800 0